A deep bore splits because of the wire, not the die. An ultra-deep bore fails when the incoming coil cannot absorb the centreline tensile stress of backward extrusion — which is why spheroidize annealing decides deep hole cold heading success. At YONGMAO, a custom fastener manufacturer in China cold heading since 1993, we treat the wire as the first tool in the stack: lamellar pearlite at 160–200 HV tears, while a spheroidized carbide structure for severe backward extrusion at 120–160 HV flows.
Three numbers separate a running job from a scrapped one: ≥85% spheroidization, a 120–160 HV hardness band, and ≥50% reduction of area. Miss one and a 20:1 bore-depth-ratio part will show chevron cracks at the bore root long before the punch wears. Below: the failure mechanism, the annealing window by grade, and the three shop-floor checks that catch a bad coil before anyone pays for heading tooling.
Published: November 2026 | By YONGMAO Engineering Team, Changzhou Yongmao Special Fastener Co., Ltd.
1. What actually splits a deep-hole blank: the punch or the pearlite?
The pearlite does. Backward extrusion pushes metal up around a punch at 800–2,000 MPa. The outer wall flows in compression, but the material at the bore centreline sits in a weak hydrostatic field and sees a net tensile stress. That is where the V-shaped chevron crack starts — invisible from outside, obvious after sectioning. Counter-intuitively, running too low a reduction makes it worse: below roughly 20–25% area reduction the centre never builds enough hydrostatic pressure, while above 70–75% the load exceeds what a medium-carbon wire can carry.
The wire microstructure decides whether that tensile field is survivable. In as-rolled lamellar pearlite, each cementite plate is a stress raiser. Japanese cold-forging research on medium-carbon steel with incomplete spheroidization found that cold cracks initiate from voids formed at cementite particles just below the bulged free surface of an upset specimen — not at inclusions, and not at the die corner. Replace those plates with rounded carbides dispersed in ferrite and the void nucleation sites largely disappear. This is why YONGMAO specifies a spheroidized carbide structure for severe backward extrusion as a microstructural requirement, not a heat-treatment adjective.
Deep-hole geometry amplifies every weakness. Three limits we check on an OEM drawing before quoting:
• Bottom thickness: ≥1–1.5× wall thickness, or the base punches through before the wall finishes filling.
• Knock-out length: a solid die punch is limited to about 8× shank diameter; longer bores need a staged route.
• Slenderness + upset strain: single-blow free upsetting stops near L/D 2.3 (two blows 4.5, three blows 8); the empirical upset-strain ceiling of about 1.6 rises only when the wire is properly spheroidized.
• Reference part: an M16 × 320 mm hollow slender shaft is a validated production case on our line, made with the patented cold extrusion elongation die for ultra-deep-hole slender parts (CN110434186B).
Three incoming checks catch a marginal coil before it reaches a multi-station header. Ask any supplier for all three, per lot:
✅ Upset test: compress cut slugs to 1/2 and 1/3 of original height; no surface fissure at 1/3 height under 10× magnification.
✅ Torsion turns + tensile: reduction of area ≥50–55%, yield-to-tensile ratio ≤0.70; a falling twist count tracks poor spheroidization faster than hardness does.
✅ Metallography + surface: spheroidization rating ≥85% with a micrograph, total decarburization ≤0.12 mm on wire ≤15 mm, surface defects ≤0.05 mm, oxygen ≤15 ppm and hydrogen ≤2 ppm.
✅ Bottom line: Deep-bore splits start at the wire's carbide morphology, not at the punch — verify spheroidization before you blame die geometry.
2. Which annealing window and wire-rod gates belong on the purchase order?
A measurable window, never the word "annealed". Most RFQs bury cold heading wire rod quality requirements spheroidize annealing in one tick-box, which lets a coil softened at the wrong temperature pass inspection. Split it into four measurable gates — temperature, soak, controlled cool, and resulting hardness — and tie each to the grade on the MTR.
Working windows for the grades we run most often (furnace-cool below 550 °C before air cooling):
• SWRCH10A / 1018 low carbon: 680–720 °C for 4–6 h → 80–110 HV, spheroidization ≥85%.
• SWRCH18A / 22A: 690–730 °C for 5–8 h → 90–130 HV, spheroidization ≥85%.
• SWRCH35K / 10B21 / 1039 (8.8–10.9 grade): 720–760 °C for 6–10 h → 120–170 HV, spheroidization ≥80%.
• AISI 5140 / 4140 alloy wire: 720 °C for 6 h reaches the minimum G2/L2 rating defined in ASTM F2282; at 660 °C and 600 °C, published spheroidization trials report very poor softening regardless of starting microstructure.
That last line is the one buyers miss. A factory can honestly write "annealed" on a certificate after a 660 °C cycle that barely changed the lamellae. If the mill cannot show a hardness band and a spheroidization rating, you now know why spheroidize annealing decides deep hole cold heading success even on a perfectly built die. Anchor the clause to GB/T 6478-2015 (steels for cold heading and cold extruding, 5–60 mm wire rod) and ASTM F2282, then require the micrograph with each bulk lot.
The remaining gates are surface and lubrication, because a well-spheroidized coil still cracks if the metal cannot slide:
• Phosphate + soap coating: 1.5–3.0 g/m² film, friction coefficient 0.05–0.10; phosphate/soap systems cut cold-extrusion friction by roughly 60–80%.
• Per-pass reduction: cap near 40% on high-strength grades and add an intermediate anneal; a single 70% pass on an incompletely spheroidized wire is the classic work-hardening crack recipe.
• Documentation: MTR, upset-test result, spheroidization micrograph and grain-flow photo per lot. Yongmao keeps all four on file for our cold heading and non-standard fastener programs, including 304HC / A2-70 slender screws up to 295 mm.
✅ Bottom line: Put a hardness band and a spheroidization rating on the PO; "annealed" alone is not a verifiable incoming-wire specification.
Frequently asked questions
Q: We already buy "annealed" wire. What exactly should we ask the mill to change?
A: Ask for three records with each lot: a hardness value inside the grade band, a spheroidization rating with micrograph, and a 1/3-height upset-test result. Those three turn a heat-treatment claim into a formability claim — and that is why spheroidize annealing decides deep hole cold heading success on long bores rather than on ordinary bolts.
Q: Can a spheroidized carbide structure for severe backward extrusion be replaced by a softer grade or a larger die radius?
A: Not for deep bores. A larger entry radius reduces surface tearing, and a softer grade lowers forming load, but neither removes the cementite plates that nucleate centreline voids. The 8× shank-diameter knock-out limit and the 20–25% minimum reduction still apply, so geometry changes cannot substitute for microstructure.
Q: Do you run OEM trial lots before committing to tooling?
A: Yes. Changzhou Yongmao Special Fastener Co., Ltd. runs 300-piece trial lots from a specified coil, with DFM feedback in 2–5 days and FAI in 7–15 days. Because the die shop and the heading line are in the same plant, we can adjust the annealing window and the station sequence without restarting the supply chain.
Next step: a free formability review
Send your drawing and bore-depth ratio to YONGMAO. Our engineering team will return a free feasibility review covering wire grade, annealing window, upset ratio and a spheroidized carbide structure for severe backward extrusion specification — before you commit to tooling. We will also include our one-page cold heading wire rod quality requirements spheroidize annealing checklist, the same one used on our own incoming-coil gate.
YONGMAO quotes OEM/ODM programs factory-direct from Changzhou, with MTR and grain-flow photos per lot. Request your free deep-hole formability review.